Generic selectors
Exact matches only
Search in title
Search in content
Post Type Selectors
Search in posts
Search in pages
Filter by Categories
Case Report
Clinical research study
Current Issue
Editorial Board
Literature Review
Narrative review
Original Article
Research Article
Review Article
Short Report
Surgical techniques
Systematic Review and Meta-Analysis
Generic selectors
Exact matches only
Search in title
Search in content
Post Type Selectors
Search in posts
Search in pages
Filter by Categories
Case Report
Clinical research study
Current Issue
Editorial Board
Literature Review
Narrative review
Original Article
Research Article
Review Article
Short Report
Surgical techniques
Systematic Review and Meta-Analysis
View/Download PDF
69 (); 236-243
doi:
10.1016/j.jor.2025.07.035

Translate:

Antibacterial and antifungal effects of silver-doped multilayered yttria-stabilized zirconia and hydroxyapatite Coatings: Potential application in biomedical implants and orthopaedics

Author affiliations
BEST/CB3S, UMR CNRS 7244, Institut Galilée, Université Sorbonne Paris Nord, Villetaneuse, 93430, France
Instituto de Biotecnología, Universidad Nacional de Colombia, Bogotá, 111321, Colombia
Engineering Department, Universidad Militar Nueva Granada, Bogotá, 110111, Colombia
Escuela de pregrado, Dirección Académica, Vicerrectoría de Sede, Universidad Nacional de Colombia, Sede la Paz, Cesar, 202017, Colombia
Biodiversidad para la Sociedad Research Group, Universidad Nacional de Colombia, Sede la Paz, Cesar, 202017, Colombia
Article History
Corresponding author(s)

⁎Corresponding author: E Lorena Medina. elmedinam@unal.edu.co

Article tools · PDF & citations

Abstract

Abstract

Implant-associated infections remain a major clinical challenge in orthopedic surgery, often caused by microbial biofilms that resist conventional antibiotic treatments. Developing multifunctional coatings that combine bioactivity and antimicrobial properties is critical to improving the long-term performance of orthopedic implants.

To design and evaluate multilayered coatings that inhibit both bacterial and fungal colonization on orthopedic implant materials, while maintaining structural and chemical properties suitable for osseointegration.

Multilayer [YSZ/HAp-Ag]n coatings—composed of alternating layers of yttria-stabilized zirconia (YSZ) and silver-doped hydroxyapatite (HAp-Ag)—were deposited on titanium substrates via RF magnetron sputtering. Samples with varying bilayer numbers (n = 1, 10, 30, 50, 70) were characterized using transmission electron microscopy (TEM), Auger electron spectroscopy (AES), energy-dispersive X-ray spectroscopy (EDS), and profilometry. Antimicrobial performance was tested against Paenibacillus sp. (bacteria) and Penicillium sp. (fungus) using a colony-counting method over 136 h.

The coatings exhibited well-defined multilayer structures with homogeneously distributed Ag nanoparticles (∼100 nm) embedded in the HAp matrix. All multilayered coatings achieved complete inhibition of Paenibacillus sp.. Inhibition of Penicillium sp. was complete in samples n1, n10, and n70, while partial inhibition (61–93 %) was observed in n30 and n50, attributed to differences in surface roughness and hydrophobicity. No microbial growth was detected on any coated surface, in contrast to uncoated titanium and polystyrene controls.

[YSZ/HAp-Ag]n multilayer coatings offer dual antimicrobial activity against bacterial and fungal pathogens, making them highly promising candidates for orthopedic implant applications. Their tunable architecture, biocompatible composition, and effective prevention of microbial colonization support their use in bone-contact devices, including joint prostheses and spinal implants.

Abstract

Graphical abstract

Image 1

Abstract

Highlights

•[YSZ/HAp-Ag]n multilayer coatings were fabricated by RF magnetron sputtering with uniform AgNP distribution.•Multilayers significantly reduced bacterial and fungal growth, with full inhibition in selected configurations.•Surface topography and wettability influenced the antimicrobial performance and colony morphology.•n30 coatings maintained MC3T3-E1 viability >70 % and exhibited the highest ALP activity, demonstrating that osteoblasts can grow on AgNP-containing surfaces without cytotoxic or morphological effects.•Multilayers combine antimicrobial efficacy and osteoblast compatibility.

Disclaimer:
This article was originally published by Reed Elsevier India Pvt. Ltd. and was migrated to Scientific Scholar after the change of Publisher.
1

1 Introduction

Biofilms are structured microbial communities, comprising bacteria, fungi, and other microorganisms,1,2 that adhere to a wide range of biological and abiotic surfaces, including tissues and medical devices.3 These communities are embedded in a self-produced extracellular matrix that retains enzymes, facilitates extracellular digestion in aqueous environments, and provides protection against desiccation, biocides, antibiotics, heavy metals, ultraviolet radiation, and host immune responses.1,2,3,4 Preventing biofilm formation on biomedical implants is of critical importance, as biofilms represent a primary cause of device-associated infections. Once established on biomaterial surfaces, biofilms display marked resistance to host immune defenses and conventional antimicrobial therapies, including antibiotics and biocides.5,4 Their persistence can lead to chronic infections caused by opportunistic pathogens such as Staphylococcus aureus,5,6Escherichia coli,7,6 and Pseudomonas aeruginosa,8,6 often resulting in severe complications and, in some cases, mortality.9 Consequently, the development of effective strategies to prevent biofilm formation is essential to enhance implant safety, functionality, and patient quality of life. The World Health Organization has identified antimicrobial resistance as a global health crisis, warning that deaths caused by resistant infections could exceed 50 million annually by 2050 if left unaddressed.10 Current strategies to mitigate biofilm-related infections include the controlled release of antibiotics and antifungals,6,3,4 as well as the surface modification of implants through the incorporation of metallic nanoparticles to inhibit microbial adhesion.4 Among these, silver nanoparticles (AgNPs) have demonstrated broad-spectrum antimicrobial activity against bacteria, viruses, fungi, protozoa, and biofilms,11 primarily attributed to the release of Ag+ ions. These ions disrupt microbial cell integrity, interfere with vital cellular functions, and ultimately lead to cell death.6

The proposed antimicrobial mechanisms of AgNPs include: (i) the release of Ag+ ions, which penetrate microbial membranes and damage DNA and essential enzymes; (ii) the generation of reactive oxygen species (ROS), inducing oxidative stress and cellular damage; and (iii) direct interaction with microbial membranes, causing structural disruption and loss of viability.6,12 However, the specific mechanisms of action may vary depending on the microbial species and physicochemical properties of the nanoparticles and remain the subject of ongoing investigation.13,14

Based on these properties, this study employed AgNPs as a doping agent to modify implantable surfaces and investigated their antimicrobial efficacy against Paenibacillus sp. and Penicillium sp. Paenibacillus sp. is a Gram-positive, spore-forming bacterium,15,16 known for its resilience under environmental stress.16 Although traditionally regarded as an environmental microorganism, Paenibacillus has been implicated in clinical infections associated with medical implants, including cardiac and breast devices,17,18 highlighting its clinical relevance. Penicillium sp., is a filamentous fungus19 characterized by rapid colonization through conidial dispersal.20 Documented cases of implant-related infections involving Penicillium sp., particularly in immunocompromised individuals, have been reported in association with prosthetic hips and breast implants.21,22 These species were selected as representative microbial models for evaluating the antimicrobial efficacy of the coatings developed in this study. Beyond microbial colonization,12 metallic implants are also susceptible to challenges such as corrosion23,24,25,26 and suboptimal surface compatibility.27,28 Corrosion by-products can elicit inflammatory responses23,29 and contribute to mechanical degradation and eventual implant failure.30,31 To address these issues, ceramic coatings have been employed as protective barriers.32 Among ceramic materials, yttria-stabilized zirconia (YSZ) is distinguished by its superior hardness, fracture toughness, and chemical stability.33,34 Meanwhile, hydroxyapatite (HAp) is widely used due to its chemical similarity to natural bone, which promotes biocompatibility and osteointegration.35,36 However, HAp is limited by its low mechanical strength and susceptibility to degradation. To enhance its properties, this study proposes the development of nanostructured multilayer coatings consisting of alternating layers of YSZ and Ag-doped HAp, deposited on titanium substrates with a nanometric alumina adhesive interlayer. The multilayered architecture disrupts the columnar grain growth typically observed in monolayer coatings, thereby reducing crack propagation, enhancing hardness, improving resistance to corrosion and wear, and decreasing roughness in the surface. In this study, multilayer systems of the form [YSZ/HAp-Ag]n were fabricated, where n denotes the number of bilayers (each comprising one layer of YSZ and one of HAp-Ag), with n values of 1, 10, 30, 50, and 70. As n increases, grain size decreases (while total coating thickness remains constant), thereby modifying structural attributes such as surface wettability, which in turn may influence microbial adhesion and biofilm formation. Accordingly, the objective of this study is to design and evaluate the antimicrobial performance of [YSZ/HAp-Ag]n multilayer coatings as a multifunctional surface modification strategy, aiming to enhance both the mechanical integrity and biological response of biomedical implants.

The development of [YSZ/HAp-Ag]n multilayer coatings presents a promising multifunctional approach for enhancing the performance of biomedical implants. By combining the mechanical robustness of YSZ with the bioactivity of HAp and the antimicrobial efficacy of silver nanoparticles, these coatings address key challenges associated with implantable materials, including microbial colonization, corrosion, and limited biocompatibility. The nanostructured multilayer design not only improves structural and surface properties but also provides sustained antimicrobial protection, thereby reducing the risk of device-associated infections. These attributes are particularly relevant in clinical settings, where implant failure due to infection and mechanical degradation remains a major concern. Therefore, the proposed coatings demonstrate significant potential for translation into real-world biomedical applications, contributing to improved implant longevity, patient safety, and overall clinical outcomes.

2

2 Materials and methods

2.1

2.1 Synthesis and characterization

2.1.1

2.1.1 Sample preparation

Commercial α-titanium discs (ASTM Grade 1, CAS 7440-32-6), 12.7 mm in diameter and approximately 1.32 mm in thickness, were employed as substrates. The discs were sectioned using wire electrical discharge machining with a molybdenum wire, then polished to a mirror finish. Subsequently, the samples were ultrasonically cleaned in ethanol and isopropanol for 10 min to remove surface contaminants.

2.1.2

2.1.2 Coating deposition

Thin film coatings were deposited using RF magnetron sputtering in a Kurt J. Lesker vacuum chamber. Two 4” targets of 99.9 % purity were employed: yttria-stabilized zirconia (YSZ, 8 % Y2O3) and hydroxyapatite (HAp). The HAp target was doped by embedding six silver inserts into the erosion zone. Titanium substrates were positioned 5 cm from the targets during deposition. An initial alumina (Al2O3) adhesion layer was deposited at 450 W and 250 °C for 15 min, under a pressure of 2 × 10−2 mbar, resulting in a thickness of approximately 20 nm. Following this, multilayer [YSZ/HAp-Ag]n coatings were deposited with n = 1, 10, 30, 50, and 70 bilayers. Each bilayer consisted of one layer of YSZ followed by one layer of Ag-doped HAp. The total thickness was kept constant across all samples. Deposition of each material was carried out at 400 W and 200 °C, using an argon flow of 50 sccm and a chamber pressure of 1 × 10−2 mbar.

2.1.3

2.1.3 Physicochemical and biological characterization

2.1.3.1
2.1.3.1 Auger Electron Spectroscopy (AES)

AES analysis was conducted using an Omicron NanoTechnology© Auger spectrometer. Prior to analysis, samples were pre-cleaned to eliminate residual surface contaminants. Data acquisition and peak assignment were performed using CasaXPS© software.

2.1.3.2
2.1.3.2 Transmission Electron Microscopy (TEM)

High-resolution TEM imaging was carried out with a JEOL JEM–2200FS + Cs© microscope operating in scanning transmission electron microscopy (STEM) mode. Elemental mapping via energy-dispersive X-ray spectroscopy (EDS) and electron diffraction pattern analysis were also performed. Cross-sectional sample preparation was achieved using a JEOL JEM 9320FIB© focused ion beam system.

2.1.3.3
2.1.3.3 Surface roughness

Surface topography was assessed using a 3D Alicona© optical metrology system, following the ISO 21920–2:2021,37 ISO 16610–21:2011,38 and ASME B46.1–202239 standards. The arithmetic mean height (Sa) was calculated from the generated surface height maps.

2.1.3.4
2.1.3.4 Contact angle

Wettability was evaluated by measuring the static water contact angle (WCA) using a Krüss DSA CA© goniometer. A 0.5 μL droplet of ultrapure filtered water was deposited onto each coated surface.

2.1.3.5
2.1.3.5 MC3T3-E1 cell culture and assays

MC3T3-E1 osteoblasts (P3–P5) were cultured in α-MEM supplemented with 10 % FBS, 1 % penicillin-streptomycin, and 1 % L-glutamine. Cells were seeded onto [YSZ/HAp-Ag]n coatings (n = 1, 10, 30, 50, 70) and incubated at 37 °C with 5 % CO2. Cell viability was assessed via the MTT assay at 24 h, 3, and 7 days, following ISO 10993–5:2009. Alkaline phosphatase (ALP) activity was measured at 7 and 14 days using p-nitrophenyl phosphate and normalized to total protein content by Bradford assay.

2.2

2.2 Antimicrobial assays

2.2.1

2.2.1 Bacterial culture and sample inoculation

Paenibacillus sp. was sourced from the Strain and Gene Bank (IBUN, Universidad Nacional de Colombia) and preserved at −80 °C in Luria Bertani (LB) broth supplemented with 40 % glycerol. For reactivation, the bacterium was cultured in LB broth (tryptone 5 g/L, yeast extract 5 g/L, NaCl 5 g/L, pH 7.2) at 30 °C under agitation (120 rpm) for 5 days. The culture was then transferred to nutrient broth and incubated until reaching a concentration of 9 × 108 CFU/mL, according to the McFarland standard. This suspension was diluted to 1.5 × 103 CFU/mL for subsequent inoculation. A total of 21 samples were inoculated (1 mL/sample), distributed across five experimental groups corresponding to n = 1, 10, 30, 50, and 70, as well as two positive controls: polystyrene and uncoated titanium. Each group was tested in triplicate and incubated at 37 °C ± 1 °C for 16 h. Post-incubation, 1 mL of 0.8 % saline solution was added to each sample, followed by 3 min of agitation to obtain the initial solution (C0). Serial dilutions (10−1 and 10−2) were prepared, and 20 μL aliquots were plated in duplicate onto nutrient agar in 15 mm wells. Plates were incubated at 37 °C ± 1 °C for 5 days. Colony-forming units (CFU) were enumerated at 16, 20, 43, and 136 h (Fig. 1).

Procedure for Paenibacillus sp. growth on control and [YSZ/HAp-Ag]n coatings.
Fig. 1 Procedure for Paenibacillus sp. growth on control and [YSZ/HAp-Ag]n coatings.
2.2.2

2.2.2 Fungal culture and sample inoculation

Penicillium sp., was stored at −80 °C in 20 % glycerol. Conidia were harvested and suspended in a 0.1 % Tween 80 solution to a final concentration of 4.16 × 107 conidia/mL. This suspension was diluted to 1.5 × 103 conidia/mL for inoculation. The assay mirrored the bacterial protocol: 21 samples (1 mL/sample) were divided into five coating groups and two positive controls; each tested in triplicate. Samples were incubated at 25 °C ± 1 °C for 16 h. Following incubation, each sample was transferred to 1 mL of 0.1 % Tween 80 solutions and agitated for 3 min to yield the initial solution. Dilutions of 10−1 and 10−2 were prepared, and 20 μL from each dilution was plated in duplicate onto potato dextrose agar (PDA) in 30 mm wells. The plates were incubated at 25 °C ± 1 °C for 5 days. CFU counts were performed at 16, 20, 43, and 136 h (Fig. 2). Fungal load (CFU/mL) was quantified using the micro-drop technique (Equation (1)), and antifungal activity was determined using Equation (2).11

Procedure for Penicillium sp. growth on control and [YSZ/HAp-Ag]n coatings.
Fig. 2 Procedure for Penicillium sp. growth on control and [YSZ/HAp-Ag]n coatings.

Equation (1). Micro-drop technique for CFU/mL quantification(1)CFUmL=x‾coloniescountedvolumeplanted(mL)dilutionfactor

Equation (2). Antifungal activity, where Nc = colony count on control and Ns = colony count on coated surface:(2)Antimicrobialactivity%=Nc−NsNc100

2.3

2.3 Statistical analysis

All experiments were performed in triplicate. Data were analyzed using one-way analysis of variance (ANOVA), followed by post hoc comparisons. A p-value <0.05 was considered statistically significant. The Shapiro–Wilk, Anderson–Darling, and Lilliefors tests were employed to assess the normality of the data distribution.

3

3 Results and discussion

3.1

3.1 Synthesis and characterization

[YSZ/HAp-Ag]n multilayer coatings were fabricated via sequential RF magnetron sputtering with alternating exposure to YSZ and Ag-doped HAp targets. Deposition times were calibrated to yield a uniform thickness of 2.264 μm ± 0.006 across all configurations. The coatings exhibited high chemical stability, with no interfacial reactions observed (Fig. 3A). TEM revealed that the YSZ layers formed a nanocrystalline matrix (Fig. 3C), while the HAp-Ag layers exhibited a structural transition—from amorphous in the inner layers to nanopolycrystalline in the outer layers (Fig. 3B and E). Silver nanoparticles (∼100 nm) were uniformly embedded in the amorphous HAp matrix without agglomeration (Fig. 3A and D).

A. TEM micrograph of [YSZ/HAp-Ag]n (n = 1): YSZ base layer (dark), HAp matrix (gray), and a silver nanoparticle (blue). (B) Multilayer structure: basal YSZ, amorphous HAp-Ag with AgNP, and upper crystalline HAp-Ag layer. (C) Electron diffraction of nanocrystalline YSZ. (D) Electron diffraction of amorphous HAp-Ag. (E) Electron diffraction of nanopolycrystalline HAp-Ag.
Fig. 3 A. TEM micrograph of [YSZ/HAp-Ag]n (n = 1): YSZ base layer (dark), HAp matrix (gray), and a silver nanoparticle (blue). (B) Multilayer structure: basal YSZ, amorphous HAp-Ag with AgNP, and upper crystalline HAp-Ag layer. (C) Electron diffraction of nanocrystalline YSZ. (D) Electron diffraction of amorphous HAp-Ag. (E) Electron diffraction of nanopolycrystalline HAp-Ag.

Electron diffraction confirmed FCC silver rings (Fig. 3D), indicating metallic Ag presence, with no evidence of incorporation into the YSZ lattice. SEM-EDS (Fig. 4) confirmed homogeneous Ag distribution, localized within HAp layers, while YSZ (dark contrast) served as structural barriers.

Cross-sectional SEM-EDS image of [YSZ/HAp-Ag]n (n = 10), showing uniform AgNP distribution.
Fig. 4 Cross-sectional SEM-EDS image of [YSZ/HAp-Ag]n (n = 10), showing uniform AgNP distribution.

Auger and EDS revealed Ag surface concentrations of 1.6-3.4%, ruling out contamination. The Ca/P molar ratio of 1.67 indicated stoichiometric HAp 37–39. Surface roughness (Sa) varied with the number of bilayers, ranging from 38.67 nm (n70) to 229.97 nm (n30) reflecting modifications in surface topography. The smoother surface observed in n70 may result from gradual surface leveling during prolonged deposition. Surface roughness influenced wettability: all coatings exhibited hydrophobic behavior (contact angle > 90°), with the lowest angle (101.9°) observed for n30 (Fig. 5). The higher roughness of this group increased wettability, consistent with Wenzel's model, which posits that surface microtextures enhaces liquid-solid interactions 40,41.

Contact angle of titanium substrate samples and multilayer systems [YSZ/HAp-Ag]n.
Fig. 5 Contact angle of titanium substrate samples and multilayer systems [YSZ/HAp-Ag]n.

Cell viability assays showed that all coatings supported MC3T3-E1 cells at 24 h, with some exceeding 100 % due to enhanced mitochondrial activity. Only n30 maintained viability above the 70 % cytotoxicity threshold across all time points, per ISO 10993–5:2009. For osteogenic differentiation, n30 and n70 showed the highest ALP activity at day 7, outperforming Ti and controls, followed by a physiological decrease at day 14. Peak ALP activity in n30 (8.5 nmol/min·μg·cm2) indicates a favorable osteogenic environment without silver-induced cytotoxicity.42,43,44

3.2

3.2 Antibacterial activity of [YSZ/HAp-Ag]n against Paenibacillus sp

After 136 h of incubation, Paenibacillus sp. growth was observed only on the polystyrene controls. All coated samples (n1, n10, n30, n50, n70) exhibited complete inhibition, with no bacterial colonies detected at any dilution level. In contrast, control samples reached 5000 CFU/mL at 20 h, as quantified using the micro-drop method (Equation (1)), confirming the antibacterial efficacy of Ag-doped coatings. Significant differences (p = 0.0037) were observed, despite non-normal data distribution. Replicates and J-shaped data distribution confirmed antimicrobial efficacy.

These results demonstrate the effectiveness of [YSZ/HAp-Ag]n multilayers in preventing bacterial colonization. Complete inhibition of Paenibacillus sp. after 136 h aligns with previous findings by Kalishwaralal et al.,45 who reported >95 % inhibition of Pseudomonas aeruginosa and Staphylococcus epidermidis biofilms using biosynthesized AgNPs. Although the bacterial strains differ, both studies underscore the broad-spectrum activity of AgNPs against Gram-positive and Gram-negative species, reinforcing their clinical relevance.

3.3

3.3 Antifungal activity of [YSZ/HAp-Ag]n against Penicillium sp

The antifungal performance of [YSZ/HAp-Ag]n coatings was evaluated using a 1.5 × 103 conidia/mL inoculum of Penicillium sp., incubated for 136 h. Fungal growth was quantified by direct colony counting. In cases where colonies exceeded 100, an estimated value of 100 CFU was assigned for comparison purposes. Table 1 summarizes colony counts, and CFU/mL values (Equation (1)) are presented in Fig. 5.

Table 1 Average colony counts of Penicillium sp. after 136 h.
Sample Colonies C0 Colonies −1 Colonies−2
Control 69,5 47,5 3
Ti 68 8,5 0,67
n1 0 0 0
n10 0 0 0
n30 27,17 2,5 0,33
n50 4,67 0,67 0
n70 0 0 0

Polystyrene and titanium controls showed high fungal proliferation, indicating minimal intrinsic antifungal activity. Coatings n1, n10, and n70 exhibited complete inhibition, while n50 and n30 showed moderate and partial inhibition, respectively. Statistically significant differences were observed (p = 0.00003164), with CFU/mL values of 233 (n50) and 1358 (n30) compared to 3475 (polystyrene) and 3392 (titanium). Antifungal activity was calculated using Equation (2).11 Results (Fig. 6) confirmed 100 % inhibition for n1, n10, and n70. Inhibition rates for n50 and n30 were 93 % and 61 %, respectively, while titanium achieved only 2.4 %. At lower conidial concentrations (10−1 and 10−2), inhibition improved across all groups. Titanium reached inhibition rates of 82.1 % and 77.8 %, while multilayered coatings consistently maintained high antifungal activity (>98 %).

CFU/mL of Penicillium sp. on [YSZ/HAp-Ag]n, control and titanium (mother solution at 136 h). Inset shows fungal growth on n30 for undiluted, 10−1, and 10−2 samples.
Fig. 6 CFU/mL of Penicillium sp. on [YSZ/HAp-Ag]n, control and titanium (mother solution at 136 h). Inset shows fungal growth on n30 for undiluted, 10−1, and 10−2 samples.

These results underscore the antifungal potential of [YSZ/HAp-Ag]n coatings in biomedical settings. Inhibition averaged 91 % at high conidial loads and increased to 98 % under diluted conditions. These outcomes align with prior reports,46 where biosynthesized AgNPs achieved 85–90 % inhibition of Candida albicans biofilms (IC50 = 0.089 ppm). Colony morphology parameters (area, diameter, circularity, and angular orientation) were analyzed using stereomicroscopy and ImageJ (Fig. 7). At lower inoculum levels, colonies were larger and less numerous, likely due to reduced nutrient competition.47

Antimicrobial activity (%) of [YSZ/HAp-Ag]n and titanium.
Fig. 7 Antimicrobial activity (%) of [YSZ/HAp-Ag]n and titanium.

Coatings n30 (7.4 mm2Fig. 8C) and n50 (135.5 mm2Fig. 8D) exhibited fewer but larger colonies compared to controls (0.5 mm2 for polystyrene Fig. 8A, 1.3 mm2 for titanium Fig. 8B), with statistically significant differences (p = 0.0341). Colonies on n50 were also less circular, suggesting that AgNPs reduced viable conidia, allowing surviving spores to expand more freely. The relatively lower effectiveness of n30 may be associated with its greater surface roughness and increased hydrophilicity, factors known to promote spore adhesion.

Morphology of Penicillium sp. colonies (mother solution, 136 h). (a) Polystyrene control, (b) Titanium control, (c) n30, (d) n50.
Fig. 8 Morphology of Penicillium sp. colonies (mother solution, 136 h). (a) Polystyrene control, (b) Titanium control, (c) n30, (d) n50.

Comparative studies have shown that Penicillium sp. colonies on CREA medium can reach diameters of 13.4–23.8 mm (141–445 mm2),48 and up to 86 mm after 14 days on Sabouraud and PDA media.49 The smaller colony areas observed here are likely due to AgNP-mediated inhibition and the influence of substrate surface properties.

Circularity analysis revealed no statistically significant differences (p = 0.255). All colonies retained a roughly circular shape, consistent with the typical morphology of Penicillium colonies, which varies according to medium and environmental factors.50 No significant differences were detected in angular orientation, and all colonies maintained symmetrical growth regardless of treatment. Despite the demonstrated antimicrobial efficacy, limitations exist. Only two microbial strains were tested under static conditions, which do not fully replicate physiological environments involving dynamic fluid flow, host proteins, and immune responses. Additionally, the specific antimicrobial mechanisms of silver against Paenibacillus sp. and Penicillium sp. remain to be elucidated, and the release kinetics of Ag+ ions were not quantified.

While the antimicrobial efficacy of [YSZ/HAp-Ag]n coatings against both Gram-positive bacteria and filamentous fungi has been clearly demonstrated, the underlying molecular mechanisms driving microbial inhibition remain to be fully elucidated. It is hypothesized that Ag+ ion release plays a central role, yet the kinetics and spatial distribution of ion diffusion within the multilayered matrix were not quantified in this study. Additionally, the interaction of these ions with microbial membranes, enzymes, and DNA, particularly in the context of multilayer surface properties such as roughness, charge, and hydrophobicity, warrants further investigation through high-resolution surface characterization and omics-based microbial profiling. Furthermore, although the current results were obtained under controlled in vitro conditions, future studies should incorporate dynamic flow systems or ex vivo tissue models to better simulate clinical environments. Addressing these aspects will be essential for advancing the translational potential of AgNP-based coatings toward next generation anti-infective biomaterials.

4

4 Conclusions

The [YSZ/HAp-Ag]n multilayer coatings, fabricated via controlled RF magnetron sputtering and incorporating uniformly distributed silver nanoparticles (∼100 nm), demonstrated potent and broad-spectrum antimicrobial activity against Paenibacillus sp. and Penicillium sp. Compared to conventional surfaces such as titanium and polystyrene, the multilayer coatings significantly inhibited microbial proliferation, particularly in the n1, n10, and n70 configurations. These results strongly suggest that the incorporation of AgNPs within a nanostructured multilayer architecture generates a microenvironment that is inherently hostile to microbial adhesion and survival—most likely through localized and sustained release of Ag+ ions that disrupt cellular structures and metabolic functions. Beyond complete growth inhibition, the coatings also altered microbial dynamics in partially active systems (n30 and n50), reducing colony density while increasing individual colony size—an effect likely mediated by the interplay between surface roughness, wettability, and resource competition. These findings highlight the importance of fine-tuning not only the chemical composition but also the physicochemical properties of the coatings to optimize antimicrobial performance. While colony morphology (e.g., circularity, orientation) remained largely unchanged, the substantial suppression of both bacterial and fungal viability indicates that [YSZ/HAp-Ag]n coatings can serve as both passive and active barriers to biofilm formation. Their dual-action antimicrobial efficacy, independent of conventional antibiotics or antifungals, makes them especially promising for clinical applications where infection risk is compounded by multidrug-resistant pathogens. The modular nature of the multilayer system enables precise adjustment of coating architecture offering a versatile platform for engineering smart surfaces with tunable antimicrobial activity, mechanical integrity, and biocompatibility. Among the multilayers tested, the [YSZ/HAp-Ag]n coating consistently supported MC3T3-E1 viability and promoted early osteogenic differentiation, with no evidence of cytotoxicity or inhibition by silver content. As such, [YSZ/HAp-Ag]n coatings hold strong potential for translation into biomedical implants across dental, and cardiovascular fields, where reducing device-associated infections is critical for long-term clinical success.

CRediT authorship contribution statement

E Lorena Medina: Conceptualization, Formal analysis, Investigation, Methodology, Validation, Writing – original draft, and, Writing – review & editing. J.J. Vaca-González: Formal analysis, Investigation, Validation, and, Writing – review & editing. L.E. Sánchez-Rey: Investigation, Methodology, Validation, Writing – review & editing. Nubia Moreno-Sarmiento: Supervision, Funding acquisition, and. Salah Ramtani: Supervision, Funding acquisition, and. Celine Falentin- Daudre: Supervision, Funding acquisition, and. Diego Garzón-Alvarado: were, Supervision, Funding acquisition, and.

Ethical approval

This study did not involve human participants or animal subjects. All experiments were performed in vitro using established microbial strains and the MC3T3-E1 osteoblast cell line. Therefore, ethical approval was not required.

Funding

This research was supported by the Universidad Nacional de Colombia, the Université Sorbonne Paris Nord (CB3S UMR CNRS 7244), and the Centro de Asistencia Técnica a la Industria SENA ASTIN–SENA regional Valle del Cauca (OT AT 0265-18 A). Additional funding was provided by the Bicentennial Doctoral Excellence Scholarship Program (BPIN 2021000100003) of the Ministerio de Ciencia, Tecnología e Innovación de Colombia, and the Embassy of France in Colombia.

References

  1. , , . The biofilm matrix. Nat Rev Microbiol. 2010;8:623-633.
    [Google Scholar]
  2. , , , . Bacterial biofilms: from the natural environment to infectious diseases. Nat Rev Microbiol. 2004;2(2):95-108.
    [Google Scholar]
  3. , , , . Bacterial biofilms: a common cause of persistent infections. Sciencie. 1999;284(5418):1318-1322.
    [Google Scholar]
  4. , , , . Nanomaterials for the treatment of bacterial infection by photothermal/photodynamic synergism. Front Bioeng Biotechnol. 2023;11
    [Google Scholar]
  5. , , , . Implant infections: adhesion, biofilm formation and immune evasion. Nat Rev Microbiol. 2018;16:397-409.
    [Google Scholar]
  6. , , , , , . Antibacterial micro/nanomotors: advancing biofilm research to support medical applications. J Nanobiotechnol. 2023;21:388.
    [Google Scholar]
  7. , , , , , , . Biofilm formation and dispersal under the influence of the global regulator CsrA of Escherichia coli. J Bacteriol. 2002;184(1):290-301.
    [Google Scholar]
  8. , et al . Stratified growth in Pseudomonas aeruginosa biofilms. Appl Environ Microbiol. 2004;70:6188-6196.
    [Google Scholar]
  9. , , , , , , . Antimicrobial surfaces for implantable cardiovascular devices. Curr Opin Biomed Eng. 2022;23
    [Google Scholar]
  10. Resistencia a los antimicrobianos.
    [Google Scholar]
  11. , et al . Synthesis and investigation of antibacterial activity of thin films based on TiO2-Ag and SiO2-Ag with potential applications in medical environment. Nanomaterials. 2022;12(6):902.
    [Google Scholar]
  12. , et al . Nanotechnology-based drug delivery systems for control of microbial biofilms: a review. Int J Nanomed. Feb. 2018;13:1179-1213.
    [Google Scholar]
  13. , , , . Functional properties of ceramic-Ag nanocomposite coatings produced by magnetron sputtering. Prog Mater Sci. 2016;84:158-191.
    [Google Scholar]
  14. , , , , , . Influence of oxygen content on the antibacterial effect of Ag-O coatings deposited by magnetron sputtering. Surf Coat Technol. 2016;305:1-10.
    [Google Scholar]
  15. , , , , . Paenibacillus agricola sp. nov., isolated from agricultural soil. Arch Microbiol. 2023;205:248.
    [Google Scholar]
  16. , , , , . Isolation, characterization and whole-genome analysis of Paenibacillus andongensis sp.nov. from Korean soil. J Microbiol Biotechnol. 2023;33(6):753-759.
    [Google Scholar]
  17. , , , , , . Breast implant infection due to <em>Paenibacillus residui</em> in a cancer patient. Clin Microbiol Infection. Aug. 2016;22(8):743-744.
    [Google Scholar]
  18. , , , . Uncommon septic arthritis of the hip joint in an immunocompetent adult patient due to Bacillus pumilus and Paenibacillus barengoltzii managed with long-term treatment with linezolid: a case report and short literature review. Pharmaceuticals. 2023;16(12)
    [Google Scholar]
  19. , , , , , . Biocidal and synergistic effect of three types of biologically synthesised silver/silver chloride nanoparticles. World J Microbiol Biotechnol. 2024;40:18.
    [Google Scholar]
  20. , , , , , . Novel method for assessing the protection lifetime of building coatings against fungi. Coatings. 2023;13(12):2026.
    [Google Scholar]
  21. , , . Rare presentation of breast implant infection and breast implant illness caused by penicillium species. Eplasty. 2022;22:ic9.
    [Google Scholar]
  22. , et al . Case report: rare pulmonary fungal infection caused by Penicillium digitatum: the first clinical report in China. Front Med. Jul. 2024;11
    [Google Scholar]
  23. , , , . Electrochemical corrosion of metal implants. Am J Roentgenol. Apr. 2005;184(4):1219-1222.
    [Google Scholar]
  24. , , , , , . Fretting and corrosion in modular shoulder arthroplasty: a retrieval analysis. BioMed Res Int. 2016;2016:1-7.
    [Google Scholar]
  25. , , , , , , . Corrosion and adverse local tissue reaction in one type of modular neck stem. J Arthroplast. Oct. 2015;30(10):1787-1793.
    [Google Scholar]
  26. , , , . Characterization and corrosion behavior of hydroxyapatite/zirconia composite coating on NiTi fabricated by electrochemical deposition. Appl Surf Sci. 2010;257(5):1774-1778.
    [Google Scholar]
  27. , . There is no such thing as a biocompatible material. Biomaterials. Dec. 2014;35(38):10009-10014.
    [Google Scholar]
  28. , , , , . Sol–gel deposited TiO2 film on NiTi surgical alloy for biocompatibility improvement. Thin Solid Films. Apr. 2003;429(1–2):225-230.
    [Google Scholar]
  29. , , , , , , . Enhanced wear and corrosion in modular tapers in total hip replacement is associated with the contact area and surface topography. J Orthop Res. Dec. 2013;31(12):2032-2039.
    [Google Scholar]
  30. , et al . Corrosion damage and wear mechanisms in long-term retrieved CoCr femoral components for total knee arthroplasty. J Arthroplast. Dec. 2016;31(12):2900-2906.
    [Google Scholar]
  31. , , , , . Corrosion behavior of PEO coatings formed on AZ31 alloy in phosphate-based electrolytes with calcium acetate additive. J Mater Eng Perform. Jul. 2017;26(7):3204-3215.
    [Google Scholar]
  32. , et al . The clinical implications of metal debris release from the taper junctions and bearing surfaces of metal-on-metal hip arthroplasty. Bone Joint Lett J. Jul. 2016;98-B(7):925-933.
    [Google Scholar]
  33. , , , . Sintering of partially-stabilized zirconia and partially-stabilized zirconia—hydroxyapatite composites by hot isostatic pressing and pressureless sintering. Biomaterials. 1996;17(18):1787-1790.
    [Google Scholar]
  34. , et al . Physical and electrical characterization of yttrium-stabilized zirconia (YSZ) thin films deposited by sputtering and atomic-layer deposition. J Mater Sci Mater Electron. Sep. 2018;29(18):15349-15357.
    [Google Scholar]
  35. , , . Development of cerium and silicon co-doped hydroxyapatite nanopowder and its in vitro biological studies for bone regeneration applications. Adv Powder Technol. 2018;29(11):2792-2803.
    [Google Scholar]
  36. , , . Preparation of hydroxyapatite coating on CoCrMo implant using an effective electrochemically-assisted deposition pretreatment. Mater Char. 2011;62(11):1076-1086.
    [Google Scholar]
  37. , . Principle of auger electron spectroscopy. 2021:47-50.
    [Google Scholar]
  38. , . Chapter 11 - auger electron spectroscopy. 2017:363-381.
    [Google Scholar]
  39. , . X-Ray Photoelectron Spectroscopy (XPS) and Auger Electron Spectroscopy (AES) 2014:93-132.
    [Google Scholar]
  40. , , , , . Effect of particle size and roughness on contact angle of ZnTe thin films. 2024:268-277.
    [Google Scholar]
  41. , , , , . Surface-wetting characterization using contact-angle measurements. Nat Protoc. 2018;13(7):1521-1538.
    [Google Scholar]
  42. , , , , . Enhancing antibacterial property of porous titanium surfaces with silver nanoparticles coatings via electron-beam evaporation. J Mater Sci Mater Med. 2022;33(7):57.
    [Google Scholar]
  43. , et al . Antimicrobial TiO2 nanocomposite coatings for surfaces, dental and orthopaedic implants. Chem Eng J. 2021;416
    [Google Scholar]
  44. , et al . Multifunctional nanocoating for enhanced titanium implant osseointegration. Colloids Surf B Biointerfaces. 2023;232
    [Google Scholar]
  45. , , , , , . Silver nanoparticles impede the biofilm formation by Pseudomonas aeruginosa and Staphylococcus epidermidis. Colloids Surf B Biointerfaces. Sep. 2010;79(2):340-344.
    [Google Scholar]
  46. , , , , , , . Effect of silver nanoparticles on Candida albicans biofilms: an ultrastructural study. J Nanobiotechnol. 2015;13(1):91.
    [Google Scholar]
  47. , et al . Conidia fusion: a mechanism for fungal adaptation to nutrient-poor habitats. J Fungi (Basel). Jul. 2023;9(7)
    [Google Scholar]
  48. , , , , . Differentiation of Penicillium roqueforti from closely related species contaminating cheeses and dairy environment. Fermentation. 2021;7(4)
    [Google Scholar]
  49. , et al . A new cytotoxic sesquiterpene Quinone produced by Penicillium sp. F00120 isolated from a deep Sea sediment sample. Mar Drugs. Jan. 2012;10(1):106-115.
    [Google Scholar]
  50. , et al . Identification and nomenclature of the genus Penicillium. Stud Mycol. 2014;78:343-371.
    [Google Scholar]
Show Sections